Evaluating the activation energy

Also, by plotting ln(s/t) against (1/T), for a given value of N, the activation energy Q can be found from the gradient (-Q/R).The photos below are taken after creeping for one minute. The spacings between the 11th and 12th coils (in mm) are marked.

 

Plot of ln(s/t) against 1/T

It may be noted that the calculated activation energy of about 30 kJ mole-1 is approximately the value for atomic diffusion in solder, as expected.