DoITPoMS Micrograph Library Micrograph 31 and full record

Micrograph 31 and full record

Link to image file for micrograph 31
Micrograph no
31
Brief description
Cu 70, Zn 30 (wt%), partial recrystallisation - annealing twins
Keywords
alloy Link to MATTER Glossary entry for alloy, annealing Link to MATTER Glossary entry for annealing, brass Link to MATTER Glossary entry for brass, copper, metal, partial recrystallisation Link to MATTER Glossary entry for partial recrystallisation, recrystallisation Link to MATTER Glossary entry for recrystallisation, twinning Link to MATTER Glossary entry for twinning, zinc
Categories
Metal or alloy
System
Cu-Zn   Link to phase diagram
Composition
Cu 70, Zn 30 (wt%)
Standard codes
Reaction
Processing
Annealed, cold rolled 50% and annealed again for 30 minutes at 600 °C
Applications
Sample preparation
Technique
Reflected light microscopy
Length bar
400 μm
Further information
This sample was annealed and 50% cold rolled, with subsequent annealing for 30 minutes at 600 °C. This has caused partial recrystallisation to occur creating new dislocation-free grains with some annealing twins. The temperature is too low for significant grain growth preventing complete recrystallisation.
Contributor
Prof T W Clyne
Organisation
Department of Materials Science and Metallurgy, University of Cambridge
Date
25/10/01
Licence for re-use
Attribution-NonCommercial-ShareAlike 4.0 International