Micrograph 194 and full record
- Micrograph no
- 194
- Brief description
- MgO-C Refractory Brick
- Keywords
- brick
, carbon, ceramic
, composite material
, graphite
, magnesia, refractory 
- Categories
- Ceramic, Composite
- System
- MgO-C
- Composition
- MgO 50-90, C 8-37 (wt%), remainder Al, Si metal addition
- Standard codes
- Reaction
- Processing
- Natural graphite flakes are mixed with MgO aggregate, metal powder and phenolic resin binder. Bricks are pressed and heated to cure and decompose the resin before in situ firing in reducing atmosphere. The metal additions getter oxygen forming ceramic phases at high temperature so protecting the carbon from oxidation and acting as a bond improving hot strength.
- Applications
- Linings of primary steelmaking furnaces, all areas of basic oxygen furnaces and at the slag line of electric arc furnaces.
- Sample preparation
- Polished and unetched.
- Technique
- Reflected light microscopy
- Length bar
- 200 μm
- Further information
- This micrograph is of a specimen which has been pressed parallel with your nose (into the screen) during fabrication, with the bright graphite flakes appearing face on. Compare with micrograph 193.
The MgO grain is polycrystalline and porous. The anisometric microstructure means the brick properties are anisotropic and so the bricks orientation must be carefully controlled on installation. These are true composite materials using ceramic (MgO, natural graphite), metal (Si, Al additives), and polymer (phenolic resin) components. - Contributor
- Prof W E Lee
- Organisation
- Department of Engineering Materials, University of Sheffield
- Date
- 02/09/02
- Licence for re-use
Attribution-NonCommercial-ShareAlike 4.0 International- Related micrographs