Micrograph 619 and full record
- Micrograph no
- 619
- Brief description
- Tensile failure surface of a carbon fibre composite
- Keywords
- alignment, carbon, carbon fibres , CFC, composite material , epoxy , fibre , fracture , neutral axis , polymer composite, pull-out , reinforcement
- Categories
- Composite, Fracture, Polymer, Polymer composite
- System
- CCcomposite
- Composition
- Carbon fibre, epoxy resin matrix
- Standard codes
- Reaction
- Carbon fibres are produced by oxidising polyacrylonitrile in air at 230 deg C whilst applying tension, and then carbonising the product in nitrogen at 1000 deg C
- Processing
- A crude carbon fibre composite was made by laying out 40 tows of fibre, painting them with epoxy resin, compressing them in a mould, and curing them for five hours at 100-190 degrees C
- Applications
- Carbon fibre composites are used as a structural material in the aerospace and automotive industries, as well as in certain high-performance sporting equipment. They present exceptional stiffness and can be structurally optimised for particular load-bearing applications.
- Sample preparation
- The bar has been bent to failure in a three-point bending rig.
- Technique
- Scanning electron microscopy (SEM)
- Length bar
- 100 μm
- Further information
- This is from the region of the fracture surface which was in tension. The fibres show clean, brittle fracture surfaces (with no fibrillation or distortion and little distortion of the matrix) and have broken at varying lengths and hence some stick out while others have left holes in the matrix. This is indicative of fibre pull-out having occurred after an initial failure of the matrix, followed by failure of the fibres themselves. This is a toughening mechanism in fibre reinforced composites. It is also involved in composite crack stopping properties; each fibre has briefly slowed the progress of the crack by opening it up along the weak fibre-matrix interface and hence blunting the crack tip. The crack therefore advances relatively slowly, with much lateral meandering.
- Contributor
- J A Curran
- Organisation
- Department of Materials Science and Metallurgy, University of Cambridge
- Date
- 03/10/02
- Licence for re-use
- Attribution-NonCommercial-ShareAlike 4.0 International
- Related micrographs
View image alone .. in a new window
Help is available on downloading images